Why d ≪ λ — the haze limit

Rayleigh scattering, particle size, and the transparency budget.

Lesson 6 of 6 · ~8 min read

Every EMA quietly assumes the particles are much smaller than the wavelength. When the assumption fails, two things change: the "effective index" picture no longer applies, and scattering dominates the optics. In practice the symptom is haze.

Rayleigh scattering

For a small sphere (diameter d << λ), the scattering cross-section goes as

σscat ∝ d6 / λ4
(2.6.1)

The λ−4 term is why the daytime sky is blue. The d6 term is the reason the single most important lever in a transparent coating is particle size. Dropping d from 100 nm to 30 nm drops the per-particle scatter by (30/100)6 ≈ 1/1400.

Rule of thumb

Keep particles below ~λ/10 for haze well under 1% at visible wavelengths. Below ~λ/20 the particulate structure is effectively invisible and the EMA is in its sweet spot.