If a third medium is brought within a few penetration depths of a TIR interface, the evanescent field couples into it and real power tunnels through. This is frustrated TIR (FTIR).
Minimum cladding thickness
Modelled as a single exponential, intensity in the beyond-cladding medium decays as
Ileak / I0 = exp(−2 κ t), κ = (2π / λ) √((n1 sin θ)2 − n22)
(4.4.1)
For the leak to stay below a target fraction L, the cladding thickness must satisfy
tmin = ln(1 / L) / (2 κ)
(4.4.2)
Numbers that matter
At 550 nm, a BK7 → air TIR at 60°, κ ≈ 0.0074 nm−1. To keep leaks below 1% requires tmin ≈ 311 nm. For 10−4, ~622 nm. These numbers are why a well-cured sub-micron low-index laminate is enough to isolate two waveguide cores; a thin one is not.