Why an index-matched interlayer lets light escape

No TIR when n_PVB ≈ n_glass.

Lesson 2 of 5 · ~7 min read

PVB was engineered for optical transparency and mechanical bonding — its index was chosen deliberately close to glass to kill the glass / PVB Fresnel reflection. That is good for a passive laminated roof, bad for one you want to edge-light.

The collapsed TIR cone

θc = arcsin(1.48 / 1.52) ≈ 76.9°

Only rays arriving at the glass / PVB interface within ~13° of grazing are guided. The rest leak straight into the PVB after one bounce. On a 1-metre plate even a single bounce at the wrong angle stops the ray from reaching the far end.

The "but only sometimes" exception

Some premium interlayers have slightly lower n (~1.46) and some glass compositions push up to 1.54. Even those edge cases give θc ≈ 72°, not enough to edge-light at scale. The cladding is the real answer.