A low-index cladding restores guiding

Thin, low-n, high-contrast — the three requirements.

Lesson 3 of 5 · ~7 min read

The role of the cladding is to re-create a large Δn at the inside face of the glass so TIR works again.

Three requirements

  • Low n: 1.20 drops the critical angle from ~77° to ~52°, which restores the guided fraction from ~23 % to ~63 % on 1.52 glass.
  • Thin: 100 – 300 nm. Thinner than this and frustrated TIR bleeds too much into the PVB; thicker and the layer becomes mechanically visible in the laminate.
  • High-contrast interface: the cladding must bond to glass on one side and to PVB on the other without an intermediate layer that would flatten the index step.

Both-side cladding

For a two-side edge-lit stack you need cladding on both the inner and outer glass / PVB interfaces. Same requirements, repeated. Uniformity improves because rays that would have leaked out of one glass face now bounce back and contribute a second time.