The two-stage Maxwell-Garnett

Air-in-shell first, particles-in-binder second — the tool's implementation.

Lesson 2 of 5 · ~9 min read

The LRI Particle Engineering Model computes an effective coating index in two Maxwell-Garnett (MG) steps.

Step 1 — particle

Treat the hollow sphere as an air inclusion (fraction φvoid) inside a shell host (nshell):

β = (εair − εshell) / (εair + 2εshell), εparticle = εshell · (1 + 2φvoid·β) / (1 − φvoid·β)

The void fraction can run as high as ~1 as the shell thins, so for this step the particle-level porosity is not clamped at the 0.74 close-packing limit. Only the next step uses that cap.

Step 2 — coating

Now treat those hollow spheres as a particle inclusion (volume fraction f ≤ 0.74) inside a binder host (nbinder), and apply MG again:

β′ = (εparticle − εbinder) / (εparticle + 2εbinder), εcoat = εbinder · (1 + 2f·β′) / (1 − f·β′)

Return ncoat = √εcoat. The 0.74 cap comes from close-packing of identical spheres; above it the MG dilute-host assumption is unphysical and Bruggeman symmetric mixing is more appropriate (see "Packing and process porosity").

Why two stages

MG is asymmetric: it treats the first argument as host, the second as inclusion. Running it twice lets us preserve that geometry at each scale — air sits inside shells, shells sit inside binder — rather than averaging everything into one bulk mixture.