A thin film on a transparent substrate behaves as a Fabry-Pérot resonator. The transmission is the Airy formula:
δ = 2πnd/λ is the half round-trip phase. T swings between two values as δ sweeps through π: a maximum (TM) when the layer is a half-wave of that λ, a minimum (Tm) when it is a quarter-wave.
Why the extrema matter
At an extremum, cos(2δ) is exactly ±1, which eliminates one unknown from the Airy equation and leaves a closed-form inversion for the refractive index n at that wavelength — Swanepoel's core observation (1983).
Two forward curves — ideal and damped
Once the pipeline has fitted (d, Δd, σ, A, B, C, k₀, k₁), it reports two forward-model curves side-by-side. Both come from the same Airy formula, but they use different damping.
- TSimSmooth is the ideal case Δd = σ = 0 — the undamped Swanepoel prediction for a perfectly smooth, perfectly uniform film with the fitted dispersion.
- TSim is Airy averaged over 21 thickness slices in [d − Δd, d + Δd] (thickness variation) and multiplied by the scatter factor exp(−(4πnσ/λ)²) at each λ (surface roughness).
Overlay them on the measured spectrum: where TSim and TSimSmooth agree, the film behaves like a textbook Swanepoel sample. Where they diverge, the gap is exactly the Δd + σ contribution the fit absorbed. A clean TSimSmooth with a measurably wider TSim band is a well-diagnosed non-uniform film; a flat TSim far below TSimSmooth is strong scatter; the two coinciding over the whole band means the fit collapsed Δd and σ to zero — look for that result as a sanity check on nominally-smooth samples.