For a film thin enough that it contributes only a few periods of phase across the measurement band, the forward model satisfies an approximate conservation law:
n(λ) · d ≈ constant across the fit
That makes the (n, d) pair almost degenerate — many combinations fit the data equally well. The covariance matrix of the LM solution flags this: the (A, d) off-diagonal element is near ±1.
What breaks the degeneracy
- Multiple angles. The Fresnel coefficients depend on angle through sin²θ; n and d contribute differently at 50°, 65° and 75°. Three angles usually drop the (n, d) correlation below 0.9.
- Wavelength range. A UV cut-on makes the dispersion observable; a NIR tail makes the film-thin limit cleaner. Both help.
- A known d. From a step-height AFM measurement or an envelope-method thickness. Lock d, fit only (A, B, C, k0, k1).