Porous low-index pitfalls

Roughness, gradient layers, and when a single model will not fit.

Lesson 5 of 5 · ~7 min read

A porous film adds three complications a Cauchy-plus-Urbach model does not address. Fitting any of them with the wrong model gives a residual that looks small but hides systematic bias.

Three things to model explicitly

  • Top-surface roughness. A thin EMA layer of air + film at the top (fraction ≈ 0.5, thickness ~σ, the RMS roughness). Ellipsometry sees roughness as an additional effective layer, not as scattering.
  • Gradient index. Porous films can have a density profile with depth. Model as 3–5 slabs with linearly-varying n, or use a parametric gradient layer.
  • Ambient effects. Dry the sample and measure under nitrogen if the pores take up water. A 1 % humidity change can shift n by ~0.01 in a 50 %-porous film.

When to stop

If the residuals still show a systematic trend across λ after adding roughness and a gradient, the Cauchy-plus-Urbach dispersion model itself is probably too rigid. Switch to a Tauc-Lorentz oscillator for the UV edge, or let the n(λ) be a free piecewise-linear function with a smoothness prior.

Low-refractive-index coatings down to RI 1.16, overcoatable and PFAS-free, live on the low-refractive-index-coatings technology page.