A low-order Cauchy for the real part, a two-term tail for the imaginary part:
n(λ) = A + B / λ² + C / λ⁴
k(λ) = max(0, k0 + k1 / λ²)
Both are empirical; the Cauchy series captures normal dispersion away from any absorption edge. The Urbach-like k(λ) rises toward short wavelengths and is clamped non-negative so the fitter never claims gain.
Where this model is wrong
- Near an absorption edge: Lorentz / Tauc-Lorentz oscillators are needed. Cauchy-plus-Urbach underfits the transition.
- For a porous film at long λ: the Cauchy series stays well-behaved but the overall n(λ) also depends on effective-medium mixing, which can drift with ambient humidity. Dry-nitrogen purge for the measurement, or fit an EMA fraction as a free parameter.
- For a graded-index film: a single n(λ) is already the wrong hypothesis. Use a multi-slice model.