What Ψ and Δ measure

ρ = r_p / r_s = tan(Ψ)·exp(iΔ) — the ellipsometry primitive.

Lesson 1 of 5 · ~8 min read

Ellipsometry measures the complex reflection ratio ρ = rp / rs. Two real numbers come out of that complex ratio at each wavelength:

tan(Ψ) · exp(i Δ) = ρ

Ψ is the amplitude ratio; Δ is the phase shift between p and s on reflection. Together they encode everything a phase-sensitive measurement can know about the stack at that wavelength and angle.

Why ratios

Taking a ratio cancels the source intensity, detector gain, and most environmental noise. Ellipsometry is phase-referenced in a way intensity-only transmission is not — which is why the method works on films too thin or too absorbing for the envelope method.

Why multiple angles

A single (Ψ, Δ) at one λ is two numbers. A film described by Cauchy + Urbach + thickness is six (A, B, C, k0, k1, d). Measuring at multiple incidence angles multiplies the data without multiplying the parameters, which is what turns an underdetermined problem into a stable fit.