Which layers move the spectrum

Sensitivity ranking — why the top layer dominates.

Lesson 4 of 5 · ~7 min read

In any multilayer AR, not every layer contributes equally to variance. A ±5 nm shift on the outermost film can move reflectance more than a ±5 nm shift on the three layers underneath it combined. Knowing which one dominates tells you which tolerance to tighten.

Sensitivity, formally

The first-order sensitivity of reflectance to a layer parameter pi is the partial derivative

si(λ) = ∂R(λ) / ∂pi

When the perturbations are independent Gaussians with σi, first-order variance adds:

Var[R(λ)] ≈ Σi si(λ)² · σi²

Each term si² · σi² is the contribution of layer i to total variance. The MC run gives you the total; ranking the components tells you which lever matters most.

Why the outer layer usually wins

  • Highest index contrast. The outer film sees air on one side (n = 1), so its interfaces have the largest Fresnel coefficients. Phase changes in that layer rotate the biggest vectors in the admittance diagram.
  • Last stage of interference. The optical thickness of the outer layer sets the final cancellation between upstream amplitude and the air interface. Perturb it and you detune the whole stack.
  • Highest process variance. On wet coating the outer layer is often the lowest-index porous film, which carries the biggest n-tolerance of the stack.

On the reference quarter-wave the "stack" is a single layer, so it dominates by default. On a real four-layer V-coat or broadband design, running the sensitivity tool alongside the MC typically reveals that 60–80 % of total variance comes from the top layer alone.

Two consequences for engineering

  • Tighten the outer layer first. Cutting its σd or σn in half typically moves yield more than tightening all inner layers put together.
  • Pick the outer index for process capability, not just for optical ideal. An ideal n = 1.22 porous film at 2σ = 0.03 can lose to an n = 1.28 film at 2σ = 0.01.