An optimiser hands you the stack with the lowest nominal mean reflectance. The MC asks a different question: what happens to that design when the real process acts on it? The two answers rarely agree, and the gap is where most yield is lost.
The paper-optimum trap
A deep, narrow reflectance minimum looks great on a plot. In production it is a liability: the second derivative at the bottom of the bowl is what sets how fast perturbations climb back out. A design with a slightly higher minimum but a much flatter bowl can carry 2× the yield at the same tolerance budget.
Two designs, same mean
- Design A (paper optimum). Nominal R̄ = 0.40 %, σ at 550 nm = 0.25 %. Mean + 2σ reaches 0.90 %. Yield at 1.0 % spec = 70 %.
- Design B (robust). Nominal R̄ = 0.50 %, σ at 550 nm = 0.10 %. Mean + 2σ reaches 0.70 %. Yield at 1.0 % spec = 95 %.
Design A wins on the datasheet. Design B wins on the cost sheet. Which one you ship depends on whether the customer specification is on nominal performance or on parts-shipped-per-batch. In practice it is almost always the second.
The design loop with the MC in it
- Run the optimiser with the nominal merit function. Get a candidate.
- Run the MC with realistic σd and σn. Record mean, σ and yield.
- If yield is short, identify the dominant layer (previous lesson) and either tighten its process σ or change the design to reduce si.
- Re-optimise with a robust merit — mean R plus a σ penalty — rather than nominal R alone.
- Re-run the MC. Accept the design where the ±2σ envelope sits inside the spec, not where the nominal does.
What robust optimisation adds to the merit
A simple robust merit is a weighted sum of nominal and variance:
α = 1 tracks the mean-plus-one-σ performance; α = 2 tracks mean-plus-two-σ. Setting α = 2 and re-running the optimiser gives you the design with the lowest datasheet-ready worst case. It is almost never the paper optimum.