The ideal single-layer AR

n = √(n₀ nₛ), d = λ₀/(4n), and what "ideal" really buys you.

Lesson 2 of 6 · ~9 min read

Pick a film thickness that puts you in destructive interference and a reflectance notch appears. Pick the right index and the notch goes all the way to zero.

nAR = √(n0 · ns), dAR = λ0 / (4 · nAR)
(3.2.1)

The index condition comes from matching the Fresnel amplitudes at the two interfaces. The thickness is the quarter-wave condition at the target wavelength λ0.

Numbers for glass

For air (1.00) → BK7 (1.52) at 550 nm, the ideal single-layer AR has n = √1.52 ≈ 1.233 and d ≈ 111.6 nm. R(550 nm) at those values is a theoretical zero. In the Fresnel Explorer exercise you confirmed uncoated BK7 reflects 4.26%; this coating makes it disappear.

Why MgF<sub>2</sub> is not enough

MgF2 is the lowest-index solid film the industry can produce at scale, at n = 1.38. That is above the ideal 1.233, so the Fresnel amplitudes do not match and the notch bottoms at ~1.3% instead of 0%. Driving further requires either a multilayer stack (next lesson) or a sub-1.30 porous low-index material. This is where Kriya LRI coatings sit on the supply chain map.