Angle and polarisation at oblique incidence

Why broadband AR narrows at an angle.

Lesson 6 of 6 · ~8 min read

Everything above assumed normal incidence. The rest of the world does not oblige. Angles of incidence that matter in practice — displays at 45°, automotive windshields at 25°, AR / VR waveguides at tens of degrees — all shift the coating’s effective thickness and split the two polarisations.

δj(θ) = (2π / λ) · nj · dj · cos θj
(3.6.1)

The phase thickness shrinks by cos θj. The coating’s design wavelength blue-shifts at angle. For a 550 nm MgF2 AR on glass, the effective design wavelength at 45° slides to around 475 nm, and the reflectance at 550 nm nearly doubles.

s/p splitting

Rs rises faster with angle than Rp. For displays and imaging systems this difference is visible to the eye as a change in colour or contrast with viewing angle — the Colour Shift Calculator quantifies the chromatic side of this story.

What a broadband AR trades

A broadband AR at normal incidence is a broadband AR with a narrower band at angle. Multi-layer stacks claw bandwidth back at angle at the cost of more layers and tighter process control. The right design hinges on the illumination cone of the finished product — not on the bench-top measurement at 0°.