Treat the film as an exponential attenuator. A single particle removes an area πr²Qext from the beam. Many non-overlapping particles stacked in a film give Beer-Lambert:
Expressing N/A in terms of volume fraction f, film thickness L, and particle diameter d:
A 10 µm film with f = 0.02 of 100 nm SiO₂ particles in air at 550 nm — the "Qext for 100 nm in air at 550 nm" figure the tool quotes gives T directly.
Dilute-limit assumption
Beer-Lambert ignores multiple scattering and dependent scattering between near-neighbour particles. It is fine when f ≲ 0.1 and particles are well separated. At higher packing the film becomes a randomly-structured composite and you switch to radiative transfer or the coherent-potential approximation.