Ghost brightness and position vs R and d

Intensity follows R₁·R₂ almost linearly; position follows 2·d·tan θ_t. Changing the coating moves one, changing the substrate moves the other.

Lesson 2 of 5 · ~8 min read

Once you accept ghost brightness ≈ Rfront · Rback, two levers fall out: the reflectance of each surface (which you set with a coating), and the substrate thickness (which you set with mechanics). The two are nearly independent — intensity is set by the coatings, position by d.

The bare-both-sides reference

A bare BK7 slab in air gives Rfront = Rback ≈ 4.26% at normal incidence (air ↔ glass, 1.00 ↔ 1.52). The ghost intensity, as a fraction of the incident light that made the first image, is

Ighost / Iin ≈ 0.0426 · 0.0426 ≈ 0.00181 = 0.181%

That is the number Ghost Lab displays as R ≈ 0.181% for the bare-both-sides preset at 0° view, and it is the baseline every AR coating is trying to suppress.

What a quarter-wave AR does to the ghost

A single quarter-wave of MgF₂ on the front — 99.6 nm at n = 1.38 on a ns = 1.52 substrate — collapses the front-surface reflectance at 550 nm to about 1.26%. Pair it with a bare back and the product becomes

0.0126 · 0.0426 ≈ 0.000537 = 0.054%

Roughly a factor 3.4 dimmer than the bare slab — not the full kill you might hope for, because the back surface is doing most of the leaking. Coat the back too and both factors drop to ≈ 1.26%, taking the ghost to ≈ 0.016% — about 11× quieter than bare.

Angle enters twice

At oblique incidence R rises (both s- and p-polarisations climb above roughly 50°), so the ghost brightens with view angle even on a well-designed AR. The position offset Δx = 2 d tan θt also grows, so the ghost walks away from its parent image. At 30° view on the coated-front/bare-back BK7 reference, the single-bounce ghost brightness is about 0.059% — close to the 0° value because MgF₂ holds its anti-reflection well out to moderate angles, but not identical.