Trading mean R for neutral colour

The two-knob design trade: push mean R down, push ΔE up.

Lesson 5 of 5 · ~7 min read

The two numbers every AR-coating project tracks — photopic mean R and ΔE across angle — are not independent. They sit on a trade-off surface that the physics draws for you, and the Colour-Shift tool shows both knobs at once.

Lower top-layer index wins on R

The quarter-wave single-layer minimum sits at Rmin = ((nf² − ns) / (nf² + ns))² — the shallower the gap between nf² and ns, the deeper the null reaches toward zero. The ideal nf = √ns ≈ 1.233 for glass (1.52). MgF₂ at 1.38 gets you a shallow null; a 1.16-index film reaches a deep one.

  • MgF₂ (n = 1.38) quarter-wave on glass — photopic mean R ≈ 1.30%.
  • n = 1.16 quarter-wave on glass — photopic mean R ≈ 0.43%.
  • Bare glass (no coating) — photopic mean R ≈ 4.26%.

But lower R also means higher ΔE

A deeper, narrower V is also a V with more chroma — the short-wavelength and long-wavelength lobes are relatively stronger compared to the near-zero bottom. The 1.16-index quarter-wave reaches Lab ≈ (3.85, 4.01, −6.16) at normal incidence, chromatic enough that even small angle shifts push ΔE above 10. The MgF₂ variant sits at a shallower V with Lab ≈ (11.29, 2.33, −3.39) and more neutral residual colour.

Angular drift reinforces the trade: the deeper V slides a longer colorimetric distance when you tilt. For the same design (a single quarter-wave on 1.52 glass), angle shift from 0° to 45° gives:

  • MgF₂ reference stack — ΔE(0°→45°) ≈ 7.0.
  • n = 1.16 reference stack — ΔE(0°→45°) ≈ 15.6.

How multi-layer designs cheat the trade

A single quarter-wave has one knob (thickness) and one zero. A 3- or 4-layer broadband stack has many knobs, and the optimiser can land the residual R(λ) in a flat valley across the full 400–700 nm band rather than a deep V. The result is both a lower photopic mean R and a flatter spectrum — which, because it is closer to uniform, is closer to neutral grey, and shifts less under tilt.