Thickness variation and the rainbow index

Why a ±5 nm wet-coating drift reads as rainbow.

Lesson 4 of 5 · ~7 min read

A wet-coating process does not deposit a perfectly uniform layer. Across a web, a sheet, or a wafer, thickness drifts by a few nanometres, and that drift reads as colour variation — the familiar rainbow fringe on a plastic-film anti-reflection coating or on a soap bubble.

The physics is the same angle-shift physics

A quarter-wave null at 550 nm requires n·d = 137.5 nm. Change d by 10% and the null moves by 10%: from 550 nm to ≈ 500 nm (thinner) or ≈ 605 nm (thicker). The V slides left or right, exactly like it slid when you tilted — but now the cause is coating non-uniformity, not viewing angle.

A realistic wet-coating standard deviation is around ±5 nm on a 100 nm film: a 5% drift. The tool makes this concrete by evaluating the CIE pipeline at the nominal and off-nominal thicknesses and reporting ΔE between them. For MgF₂ on glass, moving from 95 nm to 105 nm gives ΔE ≈ 3.7 — in the visible-at-a-glance band.

The rainbow index

Rainbow index is the tool's compact summary of how badly a stack rainbows under real-world combined drift (both thickness non-uniformity across a sample and viewing-angle variation of the observer). It is computed as the maximum CIE 1976 u′v′ chromaticity distance across every pair of the five evaluation angles — in other words, the longest chord of the chromaticity trajectory.

RI = maxi,j √[(u′i − u′j)² + (v′i − v′j)²]

Rainbow index bands the tool labels

  • RI < 0.003 — excellent: no visible colour drift across the viewing-angle range.
  • RI 0.003–0.008 — good: subtle shift visible side by side under daylight.
  • RI 0.008–0.015 — moderate: clearly visible rainbow at oblique angles.
  • RI ≥ 0.015 — poor: pronounced rainbow across the sample.