Quarter-wave starts vs optimised thicknesses

Why λ₀/4 is the historical starting point and how DE pushes past it.

Lesson 2 of 5 · ~7 min read

Every multilayer AR textbook starts the same way. Pick a design wavelength λ0, usually 550 nm. Set each layer to one quarter-wave of optical thickness at that wavelength.

dj = λ0 / (4 · nj)
(1.2.1)

For MgF2 (n = 1.38) at 550 nm that is 99.6 nm. For a n = 1.16 low-index top layer it is 118.5 nm. For a n = 1.95 high-index layer, a quarter-wave is 70.5 nm and a half-wave (the "absentee" layer trick) is 141.0 nm. Those numbers show up everywhere below because they are the honest reference against which the optimiser is judged.

What the quarter-wave start buys

  • A guaranteed deep notch at λ0. For MgF2 on 1.52 glass, R(550 nm) collapses to about 1.26 % — down from 4.26 % bare.
  • A simple symmetric spectrum around λ0, so you know what the baseline looks like before any optimiser touches it.
  • A physically meaningful initial guess for every gradient-based or population-based search. The optimiser knows where to look.

What it does not buy

A quarter-wave single-layer MgF2 on 1.52 glass reaches a mean reflectance of 1.39 % across 450–650 nm. The spectrum rises hard outside the notch: at 400 nm, R ≈ 2.21 %; at 700 nm, R ≈ 1.60 %. The notch is deep but narrow. Making it flat and wide is what the optimiser is for.

How DE improves on it

Differential evolution does not start from the quarter-wave; it starts from uniform random thicknesses in [5, 500] nm. The quarter-wave values show up in the final design only if the physics drives the solver toward them. For a single layer on a given substrate, DE converges within a few nm of λ0/(4n). For two or more layers, DE routinely finds a design whose individual layers are nowhere near a quarter-wave but whose combined phases give a broader notch than any quarter-wave stack can.