Choosing indices and why a very low top layer widens the band

Index contrast as the broadband lever; the 1.16 top layer worked example.

Lesson 3 of 5 · ~9 min read

Thickness is one knob. Index is the other, and in a broadband AR it is the bigger one. The optimiser does not vary n continuously — it picks among the materials you check in the material panel, then searches thickness for each. So the material list you hand it defines the design space.

The matching condition and why MgF<sub>2</sub> is not enough

A single-layer AR on a substrate of index ns reaches zero at λ0 only when nAR = √(n0 · ns). For air (1.00) and BK7 (1.52) that ideal index is 1.233. MgF2 at 1.38 is the lowest solid film the industry can sputter at scale — too high. A quarter-wave of MgF2 on BK7 bottoms at about 1.26 % at 550 nm and averages 1.39 % over 450–650 nm. Not zero, not even close to it.

A 1.16 top layer reaches the floor

A quarter-wave of n = 1.16 on the same substrate — 118.5 nm — bottoms at a theoretical zero near 550 nm and averages 0.54 % across the same visible band. That is the single biggest performance gain available from a single-layer AR on glass, and it falls out of nothing more than the index matching formula.

ideal nAR = √(n0 · ns) → 1.233 for 1.00 · 1.52
(1.3.1)

Why low-index widens the band

Band width scales with the mismatch at the interfaces, not with the absolute index. A top layer matched to √(n0 · ns) drops the front-interface amplitude across all wavelengths in the band, not just at λ0. The back interface then sees less to interfere with, and the stack behaves more like a well-matched gradient than a narrow-notch resonator. Add a high-index layer underneath the low-index top (the classic L/H broadband) and the two Fresnel amplitudes cancel across a wider band because both knobs are set.

Reference numbers from the optimiser's own kernel

  • Bare BK7 at 550 nm: R = 4.26 %.
  • MgF2 quarter-wave on BK7, 450–650 nm mean: 1.39 %.
  • n = 1.16 quarter-wave on BK7, 450–650 nm mean: 0.54 %.
  • n = 1.16 λ/4 on top of n = 1.95 λ/2 absentee on BK7, 450–650 nm mean: 1.63 % — the absentee layer does nothing at 550 nm by design, so adding it does not help a single-wavelength zero. Where it does help is at non-design wavelengths, where the H-layer's phase lever bends the broadband curve.