Thickness and index errors in wet coating

What drifts, by how much, and whether it reads as random or systematic.

Lesson 1 of 5 · ~7 min read

A coating never ships at its nominal recipe. Thickness drifts because wet-film deposition rate, drying and curing shrinkage all have variance. Refractive index drifts because solids content, porosity after cure, and binder density change from batch to batch. Before you ask whether a design works, you need an honest number for how much each of those moves.

A vocabulary for errors

  • Random — fluctuates from coating to coating around a stable mean. A ±σ you measure across a long production run.
  • Systematic — the whole population sits above or below the design value. Wrong solids concentration, miscalibrated wire-wound rod, drifted oven set-point.
  • Gradient — error varies across a single sheet. Edge-versus-centre thickness on a slot-die; hot-edge non-uniformity on an oven.

Monte Carlo as the tool runs it models the random part. Systematic bias is something you catch with a measurement loop, not a simulation. The simulation tells you whether the random variance alone will already lose yield — if it will, no amount of calibration saves you.

What the tool samples

For each layer the tool draws two independent Gaussians per sample: one for thickness, one for real index. The user-facing tolerance input is interpreted as a 2σ half-width, which matches how coatings specs are usually written ("±10 nm, approximately 95 % of parts within range"):

σd = told / 2, σn = toln / 2

For the reference stack in this module — a single 99.6 nm quarter-wave MgF₂ layer (n = 1.38) on a 1.52 substrate, with told = 10 nm and toln = 0.02 — this means every drawn sample sees σd = 5 nm and σn = 0.01. Extinction k is treated as deterministic: lot-to-lot k variation is negligible compared with n variation for visible-range dielectrics.

Order-of-magnitude budget for wet coating

  • Slot-die on film: typical thickness 2σ is 3–8 % of nominal — a ~100 nm layer rarely holds tighter than ±5 nm.
  • Wire-wound rod (meter-bar) coating: 2σ of ~10–15 % is common on a mature process, worse during start-up.
  • Porous-silica top layer: n-tolerance is almost always driven by porosity, with 2σ values of 0.01–0.03 across a production campaign.