Maxwell Garnett’s 1904 paper on coloured metal films gave the first useful EMA. It treats one phase — the host — as the dominant medium, and the other as a dilute collection of inclusions that each sees essentially the host’s local field.
(εeff − εh) / (εeff + 2εh) = f · (εi − εh) / (εi + 2εh)
(2.2.1)
Solve for εeff and take neff = √εeff. The Effective Medium Calculator implements exactly this.
When MG is the right call
- One phase is clearly the matrix and the other a dilute inclusion.
- Volume fraction < ~30% so the dilute-inclusion assumption still holds.
- Scatterers are small enough (<< λ) that they act as polarisable points.
Limits
MG is not symmetric in the two phases: swapping host and inclusion gives a different answer. That is a feature when it matches reality (say, dilute metal particles in a dielectric) and a bug when it does not (near the percolation threshold, around f ≈ 1/3). For higher fractions, Bruggeman is the right next step.