AR on each surface

Coating one side halves the ghost but leaves the first-surface reflection intact. Coating both sides kills both, at a cost.

Lesson 4 of 5 · ~7 min read

Two surfaces contribute to what the user sees through an AR cover: the one closest to them and the one closest to the scene. They do different jobs, and coating decisions split naturally along that line.

Front coating kills the first-surface reflection

The first image — the bright, overlapping reflection of whatever is behind the viewer — comes off the front surface. Its intensity is Rfront. A quarter-wave of MgF₂ on BK7 at 550 nm takes that from 4.26% to about 1.26%, which the eye reads as a distinct reduction in veiling glare. This is the headline benefit of any AR coating and the one users notice first.

Back coating kills the ghost

The ghost — the dim, offset second image — depends on the product Rfront · Rback. If you coat only the front, the back is still 4.26% and the ghost brightness is 0.0126 · 0.0426 ≈ 0.054%. If you coat only the back, the front still looks like bare glass but the ghost drops to 0.0426 · 0.0126 ≈ 0.054% — the same number by reciprocity of the product.

So which side you coat changes which problem you solve. Front-only gives a clean first surface with a dimmer-but-still-visible ghost. Back-only gives a bright first surface with a faint ghost. Coat both and both problems drop together.

Coating both sides — the maths

With the same quarter-wave MgF₂ on both faces, both factors land at ≈ 1.26% at 550 nm and the ghost drops to

0.0126 · 0.0126 ≈ 0.000159 = 0.016%

That is about 11× quieter than the bare slab (0.181%) and 3.4× quieter than coating the front alone (0.054%). The first-surface reflection you actually see is still just Rfront ≈ 1.26% — the back coating does nothing for it, because no scene light has reached the back when that reflection happens.