Why residual reflection has colour

A V-shape in R(λ) is not neutral grey.

Lesson 2 of 5 · ~7 min read

A quarter-wave MgF₂ layer on glass cancels reflection at exactly one wavelength — the one for which 4·nf·d = λ. At every other wavelength, the cancellation is partial. The spectrum R(λ) is V-shaped: a sharp minimum at the design wavelength, rising on both sides toward the bare-glass 4.26%.

Grey needs a flat spectrum

For the reflected light to be neutral grey, R(λ) would have to be constant across the visible band. A V-shape is not constant. Depending on where the minimum sits, the long-wavelength and short-wavelength lobes carry different weight when the CIE integrals above run, and a* and b* come out non-zero.

Reading the reference stack

A quarter-wave MgF₂ layer (n = 1.38, d = 99.6 nm) on glass (ns = 1.52) is designed for a minimum near 550 nm. The CIE pipeline on its full spectrum under D65 returns:

  • L* ≈ 11.3 — about a quarter as bright as the bare-glass reflection (L* ≈ 24.5).
  • a* ≈ +2.3 — a faint red bias (the long-wavelength lobe contributes more weight than the short one).
  • b* ≈ −3.4 — a cooler blue bias (the short-wavelength lobe still shows up in the daylight-weighted integral).
  • Photopic mean R ≈ 1.30% — the number the tool prints as the integrated reflectance under D65.
⟨R⟩phot = ∫ R(λ) S(λ) ȳ(λ) dλ / ∫ S(λ) ȳ(λ) dλ

The eye is not the bolometer. ⟨R⟩phot weights the spectrum by the photopic response ȳ(λ), so a minimum near 550 nm (where ȳ peaks) is cheaper per joule than a minimum at the band edges. Two stacks with the same bolometric R can land at very different photopic means and, via the full x̄ and z̄ weightings, at very different a* and b*.