Brillen

Prescription spectacle lens

Hard coat, anti-reflection and easy-clean on a plastic lens

A prescription lens is a soft plastic that needs a hard coat, and most lenses also carry an anti-reflection stack and an easy-clean top layer. The hard coat is a few micrometres thick. If its index differs from the lens, light reflected at the hidden boundary between them interferes with the surface reflection and the lens shows rainbow-like fringes — worse the higher the lens index. Matching the hard coat's index to the lens removes the boundary optically.

FRONT (WORLD SIDE)BACK (EYE SIDE)Easy-clean topcoatFrontAnti-reflection stackFrontIndex-matched hard coat1–5 µm · antistatic optionLensADC n 1.50 · polycarbonate 1.59 ·polythiourethane 1.60 and 1.67 · episulfide1.74Index-matched hard coatBackAnti-reflection stackBackEasy-clean topcoatBackK4K3K1K2K1K2K3K4
Gepubliceerde Kriya-positiePassend geplaatste Kriya-positieOverige laag
Volledige lagenlijst (7)
  1. Easy-clean topcoat FrontK4
  2. Anti-reflection stack FrontK3
  3. Index-matched hard coat 1–5 µm · antistatic optionK1 · K2
  4. Lens ADC n 1.50 · polycarbonate 1.59 · polythiourethane 1.60 and 1.67 · episulfide 1.74
  5. Index-matched hard coat BackK1 · K2
  6. Anti-reflection stack BackK3
  7. Easy-clean topcoat BackK4

Werkwijze

Versie 1 · voor het eerst gepubliceerd

A hard coat with the index of the lens, a wet-coated AR stack on top, an easy-clean layer to finish.

Hoe deze coating wordt aangebracht — stappen, publieke onderbouwing en wat bij de apparaatmaker blijft.

  1. Hard coat with the index of the lens

    Solvent-free, index up to 1.65: matches polycarbonate and n 1.60 lenses and cuts the swing on n 1.67 to 5.7–6.3 %. Antistatic option: 10⁶–10¹² Ω/sq.

    Lagen: Index-matched hard coat
  2. Wet-coated AR on the hard coat

    Thin-film model: quarter-wave n 1.30 (106 nm) on half-wave n 1.95 (141 nm) on quarter-wave n ≈ 1.6 (about 85 nm), below 0.05 % luminous reflectance. Kriya's published value for multi-layer AR: R < 0.15 %.

    Lagen: Anti-reflection stack
  3. Easy-clean top layer

    Water contact angle above 100° without fluorinated chemistry.

    Lagen: Easy-clean topcoat

Publieke onderbouwing

Geselecteerde vervallen octrooien, publicaties, boeken en normen die de stand van de techniek beschrijven.

Blijft bij de apparaatmaker

Lens material, surfacing and tint.

Deze beschrijving is geen juridisch advies.

Referenties

  1. US 8,432,624 — Optical article and method for producing the same — fringes from index mismatch and thickness variation on n 1.67 and 1.74 lenses; oven cure at 125 °C
  2. US 5,165,992 — Hard coating film and optical elements having such coating film — 1991 filing: high-index oxide particles in the hard coat suppress interference fringes on high-index plastic lenses
  3. US 5,834,549 — Transparent conductive coating composition and transparent antistatic molded article — 1998 patent: UV-curable transparent coating made antistatic with conductive tin-oxide powder, for substrates such as polycarbonate
  4. H. A. Macleod, Thin-Film Optical Filters, 3rd edition (2001), chapter 3: Antireflection coatings — multi-layer designs for the visible; sections 3.4 and 3.5: coatings with two zeros, and coatings for the visible and the infrared together · link: publisher page of the current edition
  5. US 6,210,858 — Anti-reflection film and display device using the same — 1997 filing: wet-coated anti-reflection film with hard coat, high-index layer and a low-index layer (n 1.20–1.55) that owes its index to micro voids

Schematisch, niet op schaal.