AR & VR

Eye tracking through a lens

Near-infrared emitters and a camera — and every lens surface between them and the eye

Eye tracking lights the eye with near-infrared emitters, typically around 850 or 940 nm, and films it with a small camera. The tracker looks for the reflections of the emitters on the cornea, which reflects only 2.5 %. In headsets, and in glasses worn with prescription inserts, a lens sits between tracker and eye, and each of its surfaces mirrors the emitters back into the camera. A lens coated for visible light only can be worse than no coating at all.

EYE SIDETRACKER SIDEVisible + near-infrared AREye-side surface of the lensHard coatCarries the AR stackLens between tracker and eyePrescription insert or headset lens ·n 1.5–1.67Hard coatVisible + near-infrared ARTracker-side surface of the lensAirNear-infrared AR on the camerawindowEye tracker: emitters and cameraOutside the lens, looking through it · 850 or940 nm · not KriyaK1K3K3K1K2
Gepubliceerde Kriya-positiePassend geplaatste Kriya-positieOverige laag
Volledige lagenlijst (7)
  1. Visible + near-infrared AR Eye-side surface of the lensK1
  2. Hard coat Carries the AR stackK3
  3. Lens between tracker and eye Prescription insert or headset lens · n 1.5–1.67
  4. Hard coatK3
  5. Visible + near-infrared AR Tracker-side surface of the lensK1
  6. Near-infrared AR on the camera windowK2
  7. Eye tracker: emitters and camera Outside the lens, looking through it · 850 or 940 nm · not Kriya

Werkwijze

Versie 1 · voor het eerst gepubliceerd

One AR stack for the visible and the tracker's band on both surfaces of the lens; emitters and camera stay outside the lens.

Hoe deze coating wordt aangebracht — stappen, publieke onderbouwing en wat bij de apparaatmaker blijft.

  1. Hard coat on both sides of the lens

    Pencil hardness 3H+ to 4H; index matched to the lens, up to 1.65.

    Lagen: Hard coat
  2. AR for the visible and the tracker's band

    Thin-film model on n 1.52: four layers alternating n 1.30 and n 1.95, 155 / 23 / 61 / 21 nm from the air side. On average 0.8 % over the visible, 0.3 % at 850 nm, 0.55 % at 940 nm, and the lens stays transparent further into the infrared. A visible-only stack reflects about 10 % at 940 nm.

    Lagen: Visible + near-infrared AR
  3. Quarter-wave low-index layer on the camera window

    n 1.30, about 180 nm for 940 nm: 0.3 % instead of 4.3 % per surface (thin-film model).

    Lagen: Near-infrared AR on the camera window

Publieke onderbouwing

Geselecteerde vervallen octrooien, publicaties, boeken en normen die de stand van de techniek beschrijven.

Blijft bij de apparaatmaker

Emitters and their optics, the camera, where they sit and the tracking software. This stack has no emitters and no infrared combiner inside the lens.

Deze beschrijving is geen juridisch advies.

Referenties

  1. US 4,145,122 — Method and apparatus for monitoring the position of the eye — 1979 patent: infrared emitter and detector carried by a spectacle frame
  2. US 6,210,858 — Anti-reflection film and display device using the same — 1997 filing: wet-coated anti-reflection film with hard coat, high-index layer and a low-index layer (n 1.20–1.55) that owes its index to micro voids
  3. H. A. Macleod, Thin-Film Optical Filters, 3rd edition (2001), chapter 3: Antireflection coatings — multi-layer designs for the visible; sections 3.4 and 3.5: coatings with two zeros, and coatings for the visible and the infrared together · link: publisher page of the current edition

Schematisch, niet op schaal.