Eyewear

Prescription spectacle lens

Hard coat, anti-reflection and easy-clean on a plastic lens

A prescription lens is a soft plastic that needs a hard coat, and most lenses also carry an anti-reflection stack and an easy-clean top layer. The hard coat is a few micrometres thick. If its index differs from the lens, light reflected at the hidden boundary between them interferes with the surface reflection and the lens shows rainbow-like fringes — worse the higher the lens index. Matching the hard coat's index to the lens removes the boundary optically.

FRONT (WORLD SIDE)BACK (EYE SIDE)Easy-clean topcoatFrontAnti-reflection stackFrontIndex-matched hard coat1–5 µm · antistatic optionLensADC n 1.50 · polycarbonate 1.59 ·polythiourethane 1.60 and 1.67 · episulfide1.74Index-matched hard coatBackAnti-reflection stackBackEasy-clean topcoatBackK4K3K1K2K1K2K3K4
Kriya coating position — published on kriya-materials.comKriya chemistry applies — application fit from public literatureOther device layers — not supplied by Kriya
All layers (7)
  1. Easy-clean topcoat FrontK4
  2. Anti-reflection stack FrontK3
  3. Index-matched hard coat 1–5 µm · antistatic optionK1 · K2
  4. Lens ADC n 1.50 · polycarbonate 1.59 · polythiourethane 1.60 and 1.67 · episulfide 1.74
  5. Index-matched hard coat BackK1 · K2
  6. Anti-reflection stack BackK3
  7. Easy-clean topcoat BackK4

Working method

Version 1 · first published

A hard coat with the index of the lens, a wet-coated AR stack on top, an easy-clean layer to finish.

Step by step: where each layer goes, its index, its thickness and how it is cured. Compositions are not part of it. Point at a step to see its layers.

  1. Hard coat with the index of the lens

    Solvent-free, index up to 1.65: matches polycarbonate and n 1.60 lenses and cuts the swing on n 1.67 to 5.7–6.3 %. Antistatic option: 10⁶–10¹² Ω/sq.

    Layers: Index-matched hard coat
  2. Wet-coated AR on the hard coat

    Thin-film model: quarter-wave n 1.30 (106 nm) on half-wave n 1.95 (141 nm) on quarter-wave n ≈ 1.6 (about 85 nm), below 0.05 % luminous reflectance. Kriya's published value for multi-layer AR: R < 0.15 %.

    Layers: Anti-reflection stack
  3. Easy-clean top layer

    Water contact angle above 100° without fluorinated chemistry.

    Layers: Easy-clean topcoat

Public basis

Earlier public documents that describe the same steps.

Stays with the device maker

Lens material, surfacing and tint.

A working method describes how a coating can be applied. It is not legal advice. The design of a complete device, and clearing it against the rights of others, stays with the device maker.

Public references

  1. US 8,432,624 — Optical article and method for producing the same — fringes from index mismatch and thickness variation on n 1.67 and 1.74 lenses; oven cure at 125 °C
  2. US 5,165,992 — Hard coating film and optical elements having such coating film — 1991 filing: high-index oxide particles in the hard coat suppress interference fringes on high-index plastic lenses
  3. US 5,834,549 — Transparent conductive coating composition and transparent antistatic molded article — 1998 patent: UV-curable transparent coating made antistatic with conductive tin-oxide powder, for substrates such as polycarbonate
  4. H. A. Macleod, Thin-Film Optical Filters, 3rd edition (2001), chapter 3: Antireflection coatings — multi-layer designs for the visible; sections 3.4 and 3.5: coatings with two zeros, and coatings for the visible and the infrared together · link: publisher page of the current edition
  5. US 6,210,858 — Anti-reflection film and display device using the same — 1997 filing: wet-coated anti-reflection film with hard coat, high-index layer and a low-index layer (n 1.20–1.55) that owes its index to micro voids

Schematic, not to scale. Layer order, indices and thicknesses are typical values from the public references; real devices differ by maker and generation. Kriya values as published on kriya-materials.com. Kriya formulates every coating for the customer's substrate, process and specification.