Stoney 응력 & 기판 휨

What curvature does a stressed film induce in its substrate?

측정된 기판 곡률에서 등이축 박막 응력을 계산하거나, 목표 응력에 대한 웨이퍼 휨을 예측합니다. 12개의 기판 재료.

How it works

Stoney's equation relates the biaxial stress in a thin film to the curvature it induces in a much thicker substrate, given the substrate's biaxial modulus and thickness and the film thickness. The equation assumes an elastic substrate, a uniform film stress and a film-to-substrate thickness ratio below a few percent. Measured curvature therefore gives a direct read-out of residual stress for thin coatings.

Worked example

Si(100), E 130 GPa, ν 0.28, 525 µm substrate, 1 µm film, R 10 m

Inputs: substrate = silicon_100, substrateThicknessUm = 525, filmThicknessNm = 1.000e+3, radiusOfCurvatureM = 10

Result: 829.4 MPa

Reference: Stoney 1909 Proc. R. Soc. A 82, 172; Freund & Suresh 2003 §2.3

Computed by this tool's kernel at build (commit dae6663).

Validation method, references and test-case results: /validation#stoney-stress

Request accessOpen the interactive tool