과제

The glass manufacturer needed a high refractive index coating on display glass (0.7 mm) that could achieve RI 1.85 with maximum hardness. Existing HRI coatings from other suppliers could not reach 8H pencil hardness at these RI levels, and lower cure temperatures were desired to reduce energy costs.

02

접근 방법

Kriya developed three thermal-curable HRI formulation variants (V1, V2, V3), testing cure temperatures from 130°C to 200°C. Formulation optimisation focused on reducing haze through organic compound reduction (V2, V3) while maintaining RI and hardness targets. Low-outgassing variants were developed in response to customer requirements.

03

성과

V1 achieved RI 1.85 and 8H pencil hardness across all cure temperatures (130–200°C). V2 delivered the lowest haze: 0.49% at 200°C cure. All variants achieved 100% adhesion (ASTM D3359). Higher cure temperatures reduced haze significantly, with the majority of improvement occurring at 160°C.

Kriya를 선택하는 이유

Kriya’s sol-gel chemistry uniquely enables 8H pencil hardness at RI 1.85 via thermal cure alone, with tuneable cure temperatures and low-outgassing options that competitors cannot match.

핵심 지표

8HRI 1.85에서의 연필 경도
0.49%달성된 최저 헤이즈
100%밀착성 (ASTM D3359)
130°C최소 경화 온도

사용 제품

관련 응용 분야

Optical Components →

유사한 응용 상담

기술팀이 귀하의 요구사항에 이 접근 방법이 적용 가능한지 평가해 드리겠습니다.

대화 시작